资源描述
按一下以編輯母片標題樣式,按一下以編輯母片,第二層,第三層,第四層,第五層,*,材料與熱處理,金屬材料,製造一部 牛中麟 2004/2/9,1,1,材料種類,金屬,陶瓷,塑膠,複合材料,半導體,鍵結,金屬鍵,離子鍵,共價鍵,共價鍵+凡得瓦爾鍵,-,共價鍵,強度,3,1,4,2,-,耐溫性,3,1,4,2,-,導電性,1,4,3,-,2,量產性,1,2,1,3,4,加工性,1,3,1,2,3,化學安定性,3,2,1,3,2,金屬材料種類,鋼鐵,非鐵金屬與合金,鋼鐵,命名規範,美國,SAE/AISI:,前2位數字表示鋼種,後2位數字表示碳含量,4140:41表示鉻鉬鋼,40表示,0.40%C,日本,JIS:,以英文表示鋼種,後接編號或強度或元素含量,S45C:0.45%C,之碳鋼,鋼鐵的種類,碳鋼,低合金鋼,高強度低合金鋼,工具鋼,不鏽鋼,其他特殊鋼,鑄鐵,碳鋼,0.30%,C,為低碳鋼,0.300.55%,C,為中碳,0.55%,C,以上為高碳,抗拉強度、降伏強度、硬度都隨碳含量增多而增加,但伸長率、斷面縮率及衝擊值則相反,即碳愈多韌性愈低,鋼鐵之碳含量愈多則愈硬脆,碳鋼,一般構造用:,碳含量0.120.30%,直接使用,不需熱處理,機械構造用:,碳含量低於0.25%者需850950正常化處理,碳含量高於0.25%者則作正常化或者淬火(800900)+回火(550650),鑄鋼,碳5%),肥粒鐵型,沃斯田鐵型,麻田散鐵型,析出硬化型,代表鋼種,430,442,304,316,410,440,C,630,麻時效鋼,成份特徵,%Cr-17%C,13,Ni6%,%Cr-17%C,13,Al,Nb,Mo,Ti,Ta,之添加,耐蝕性,2,1,3,2,機械性質,4,4,2,1,熱處理,退火,退火,安定化,淬火+回火,固溶化+時效,用途,便宜,廣泛,低溫,化學容器,刀具,機械零件,軍事,高級零件,沃斯田鐵系不銹鋼無磁性,其他則有,不銹鋼之耐蝕性以,沃斯田鐵系的304、316最佳,且無磁性,其他特殊鋼,耐熱鋼,耐高溫氧化及具高溫強度,309、310(最高使用溫度500700),軸承鋼,彈簧鋼,磁氣用鋼,其他特殊合金鋼(例:鎂熱室壓鑄用鵝頸活塞活塞環材質1.2888),鎢鋼:唐卡龍(碳化鎢),刀具材質等級:高碳鋼,高速鋼,唐卡龍唐卡龍+鍍膜,鑄鐵,白鑄鐵,灰鑄鐵,展性鑄鐵,延性(球墨),鑄鐵,特殊合金,鑄鐵,碳之型式,雪明碳鐵,片狀石墨,不規則石墨,球狀石墨,-,特性,硬脆、耐磨,脆、易加工、吸震、滑動磨耗性佳,遠優於白灰鑄鐵之機械性質,鑄鐵中最佳之強度韌性組合,耐蝕、耐磨、耐高溫(視成份而定),應用,水泥、採礦業之滾筒、磨球,引擎本體、工具機本體,高強度機械零件,略同於展性鑄鐵,逐漸取代之,特殊零件,非鐵合金,鋁及鋁合金,鎂合金,鋅合金,鈦及鈦合金,銅及銅合金,鎳及鎳合金,錫、鉛及其合金,貴金屬金、銀、鉑,鋁合金命名規範,美國鋁業協會,日本,JIS,美國鋁業協會,鍛造用鋁合金為4位數(7075,6061),鑄造用鋁合金為3位數(,A380.1),鍛造用鋁合金代號,第1位數與主要合金成份關係,共有八個系統,1,xxx,系為純鋁,而2,xxx,至8,xxx,系為合金,第2位數字用來區分舊型合金與改良合金,通常以0代表最早開發者,而1、2、3、4、則是代表改良合金,通常指雜質含量較少的合金,第3、4位數字主要用來區別同一系統合金成份上的差別,但對純鋁而言,後兩位數字代表純度百分比小數點後兩位,7,0,75,鍛造鋁合金代號,合金系 主要合金元素,合金系 主要合金元素,1,xxx,無,2xxxCu,3xxxMn,4xxxSi,5xxxMg,6xxxMg,Si,7xxxZn,8xxx,其他,鑄造鋁合金代號,第1位數與主要合金成份關係,第2、3位數係區別同一系合金中成分上的差別,xxx.0,係表示鑄件,其成分合乎鑄件的規定,,xxx.1,與,xxx.2,則表示鑄錠,其成分合乎鑄錠的規定,在,xxx,之前加字母則用來區分雜質或微量元素的差別,如,A356,與356或,A380、B380,與380。,3,80,.1,A,鑄造鋁合金代號,合金系 主要合金元素,合金系 主要合金元素,1,xx.99%Al,2xx.Al-Cu,3xx.Al-Si-Mg,Al-Si-Cu,Al-Si-Cu-Mg,4xxAl-Si,5xxAl-Mg,7xxAl-Zn,8xxAl-Sn,日本,JIS,壓鑄鋁合金,7075為鍛造鋁合金,A380,和,ADC12,為,Al-Si-Cu,合金,純鋁,99%以上,耐蝕性、光輝、導電性、延性。,導電材料及鋁箔要求之純度為99.45%以上,Al-Cu,合金,2,xxx,系列及2,xx,系列,銅是析出硬化元素,又可減少凝固收縮孔洞以提高韌性,若添加,Mg,可進一步促進析出硬化的幅度(2,xxx,系列合金強度僅次於7,xxx,系列合金),Al-Mn(3xxx),添加1.2%,Mn,可產生,MnAl,6,而散佈強化(3003合金),再添加1%,Mg(3004,合金)可在不犧牲耐蝕性之下提高強度,廣泛使用於烹調用具、生活器具等。易開罐即為3004鋁合金。,Al-Si,合金(4,xxx,3xx,4xx),矽是最能促進鑄造性的合金元素,可使流動性好、縮孔小。此外還可提高鋁合金之剛性(複合強化)以及耐磨性,380、356等合金即為應用廣泛的高強度鑄造合金,高矽含量的390合金具有高耐磨、低熱膨脹率,因此用於滑輪、引擎汽缸、空氣壓縮機等,Al-Mg,合金(5,xxx,5xx),鎂在鋁合金中是固溶強化元素,並能保持良好的延展性及耐蝕性,並且是最適合焊接的鋁合金,適合作為車、船、建築物之結構材料(如5083、5086、5056、5456等),含鐵量少者還可得到極光亮的陽極處理皮膜,適合作外觀件(如5005、5050、5457、5657等),Al-Mg-Si,合金(6,xxx),所含的鎂及矽並不多,透過,Mg,2,Si,的析出,,T4,處理後的強度介於1530,ksi,T6,處理後則可3040,ksi,,在鋁合金中屬於中強度等級,僅次於7000及2000系合金,擠型性、耐蝕性、焊接性和陽極處理效果都不錯,因此廣泛用於建築結構材料,如門窗、欄杆等(如6061、6063等)。,Al-Zn(-Mg-Cu),合金,透過,MgZn,2,和,Al,2,Cu,的析出而成為強度最高的鋁合金,為飛機的主要結構材料(如7075、7050、7178、7079等),鋁合金熱處理代號,可熱處理合金為2,xxx、6xxx、7xxx、2xx、3xx,和7,xx,系列;其他系列則靠固溶強化和應變硬化來達到硬化的效果,在合金代號之後,可進一步連接適當的代號來表示該合金所經的加工處理或熱處理,鋁合金熱處理代號,F:,經加工成型者,O:,經退火者,H:,經應變硬化者,H1n:,僅應變硬化者,H2n:,應變硬化後經部分退火者,H3n:,應變硬化後作安定化處理者,n=2,為20%常溫加工(1/4硬質),n=4,為40%常溫加工(1/2硬質),n=6,為60%常溫加工(3/4硬質),n=8,為80%常溫加工(硬質),n=9,為90%常溫加工(特別硬質),鋁合金熱處理代號,W:,經固溶處理者,T:,熱處理者,T1:,經高溫加工成型後自然(室溫)時效至相當安定之狀態,T2:,經退火處理者(僅適用於鑄件),T3:,經固溶處理後冷加工者,T4:,經固溶處理後自然時效至相當安定狀態,T5:,經高溫加工成形後人工時效者,T6:,固溶處理後人工時效者,T7:,固溶處理後過時效處理者,T8:,固溶處理後冷加工及人工時效者,T9:,固溶處理及人工時效後再冷加工者,T10:,高溫加工成形及人工時效後再冷加工者,常用鋁合金之熱處理條件,固溶化(,T4),時效處理(,T6),溫度,C,溫度,C,時間,hr,6061,530,175,8,6063,520,175,8,擠型淬水(,T1),205(,T5),1,7075,465,120,24,壓鑄合金,?,壓鑄件氣孔多,高溫熱處理會起泡變形,鎂及鎂合金,鎂合金是最輕的實用合金,具有良好的車削性以及甚高的強度-密度比(比強度)和剛性-密度比:在相同重量下,鎂合金之撓曲度小於鋁合金、鈦合金及鋼鐵;同理,在相同剛性下,鎂合金的重量較後三者輕。,鎂合金在金屬中有最佳的吸震性。加工性極佳。,純鎂不存在於自然界中,必須以下列2種方法還原取得:(1)海水電解,(2)礦石熔煉。,鎂合金代號,鎂合金的代號是採用2個字母及2個數字的表示法,每個字母係代表一個主要元素,並依含量高低順序排列先後,數字則對應表示該元素的百分比,數字後再加上,A/B/C/D/E,表示純度,A Z 9 1 D,鋁,Al-9%,鋅,Zn-1%,高純度,鎂合金之元素代號,A,Al,鋁,M,Mn,錳,B,Bi,鉍,N,Ni,鎳,C,Cu,銅,P,Pb,鉛,D,Cd,鎘,Q,Ag,銀,E,稀土元素,R,Cr,鉻,F,Fe,鐵,S,Si,矽,H,Th,釷,T,Sn,錫,K,Zr,鋯,W,Y,釔,L,Li,鋰,Z,Zn,鋅,廠內壓鑄鎂合金為,AZ91D,主要合金元素為鋁和鋅,合金元素對鎂合金之影響,鋁:增加強度硬度(,Mg,17,Al,12,析出)、增加流動性,鋅:增加(室溫)強度硬度(,MgZn,析出)、若超過1%則會導致熱裂,錳:藉熔煉時和鐵鎳鈷銅等重金屬元素析出沈澱而提高耐蝕性、降低流動性,稀土元素:增加高溫強度、降低焊裂和氣孔,鈣:增加高溫強度、減輕鎂湯燃燒,鋰:降低強度、增加延性,矽:增加流動性、降低耐蝕性,鋯:晶粒細化,釔:增加高溫強度,鐵、鎳:降低耐蝕性,銅:降低耐蝕性、增加高溫強度,鈹:減輕鎂湯燃燒、晶粒粗大化,鋅合金,特性,在壓鑄合金中鋅的強度僅次為銅合金(高於鋁、鎂合金),熔點最低因此是最容易壓鑄的材料,再加上流動性高,適合大量生產且形狀複雜的鑄件,廠內使用之鋅合金有3種,3號(,Zn3),最廣泛使用的熱室壓鑄鋅合金,ZA8,比#3更佳的強度,但熔融溫度更高,尚可勉強適用於熱室壓鑄法,ZA27,強度最高、最耐磨以及最輕的鋅合金,必須使用冷室壓鑄法。,最廣泛使用的鋅合金為3號料,強度最高最耐磨的是,ZA27,3號鋅合金不可稱為,ZA3!,鈦及鈦合金,高熔點、高強度(接近鋼鐵材料)、低密度(4.5,g/cm3),和極優越的耐蝕性和生物親和性的諸多特性,在化工、航太、生醫方面有無可取代的用途,銅及銅合金,紅銅(純銅)導電、導熱性在金屬中排名第二,僅次於銀,使用量超越銅合金。,黃銅(銅鋅合金,brass),鋅為強化元素。銅-510%鋅用為錢幣、紀念章等。銅-30%鋅(俗稱之七三黃銅或彈殼黃銅)具有最佳的強度、延性以及加工性之組合。銅-40%鋅具有最高強度。添加錫、鉛、鋁、矽、鐵、鎳等則稱為特殊黃銅(壓鑄銅合金屬於此類),銅及銅合金,青銅(銅錫合金,bronze),錫含量從3.5%25%,另有添加磷、鉛和鋅者,此外,還有銅鋁、銅鎳、銅矽、銅鎳矽、銅錳、銅鈹(鈹銅)等合金,鎳及鎳合金,鎳鐵合金有高導磁、超低熱膨脹係數、不受溫度影響的彈性係數之特性,鎳鉻合金耐高溫氧化,可用於1100以內的高溫爐發熱體(鎳-20%鉻),超合金:高溫環境中,耐熱鋼可使用至600以下,6001000則可使用鈷基及鎳基超合金,添加鉬、鉻、銅、鐵、矽等還可用於高腐蝕性環境,廠內壓鑄合金成份(鑄錠),AZ91D,A380,ADC12,359.2,Zn3,ZA8,ZA27,Cu,0.015,3.04.0,1.53.5,0.1,0.1,0.81.3,2.02.5,Si,0.05,7.59.5,9.612,8.59.5,-,-,-,Mg,其餘,0.1,0.3,0.550.70,0.250.50,0.020.03,0.0120.02,Zn,0.450.9,3.0,1.0,0.1,其餘,其餘,其餘,Fe,0.004,1.3,1.3,0.12(0.6),0.075,0.065,0.072,Mn,0.17,0.5,0.5,0.1,-,-,-,Ni,0.02,0.5,0.5,-,-,-,-,Sn,-,0.35,0.3,-,0.002,0.002,0.002,Al,8.59.5,其餘,其餘,其餘,3.94.3,8.28.8,25.528.0,Pb,-,-,-,-,0.04,0.005,0.005,Cd,-,-,-,-,0.003,0.005,0.005,壓鑄合金物性,AZ91D,A380,ADC12,359.2,Zn3,ZA8,ZA27,密度,g/cm,3,1.81,2.68,2.74,2.67,6.64,6.3,5.0,熔點,C,470595,540595,515580,565600,382387,375404,376484,比熱,Btu/lb.F,0.25,0.23,0.23,0.23,0.10,0.104,0.125,熱傳導率,W/m.K,62,96,96,138,113,115,125,熱膨脹率,10,-6,/,K,15.2,11.7,11.5,20.9,15.2,12.9,14.4,導電率,(%,IACS),10,31,23,23,27,27.7,29.7,壓鑄合金機械性質,AZ91D,A380,ADC12,359.2,Zn3,ZA8,ZA27,降伏強度,ksi,23,23,22,30,-,42,53,極限強度,ksi,34,47,45,40,40,54,61,伸長率,%,3,3.5,3.5,3,10,610,13,硬度,HB,60,80,80,-,82,95110,105125,疲勞強度,Ksi(5e8),14,20,19,16,6.9,7.5,25,彈性模數,10,6,psi,-,10.3,10.3,10.5,-,10.2,10.3,熱處理,簡介、種類以及影響,熱處理簡介,熱處理的原理,相變態,水的3態(4態)外觀、性狀都有明顯的變化,固態材料在不同的溫度及組成下也會有不同型態(相)的轉變,即為相變態。熱處理就是對材料施以溫度、應力的控制,使材料產生相變態而變軟或變硬(不同的機械性質)以利加工、成形或使用,熱處理實例,材料:含碳量1.0%的高碳鋼,球化退火後,其微結構為肥粒鐵+球狀碳化物,硬度小於,HRc20,,可以輕易地用普通車刀、鑽頭、銑刀等予以加工,經淬火、回火後使成回火麻田散鐵後,硬度可達,HRc6062,,足以作為車刀、鑽頭及銑刀等切削工具,(我為刀俎,人為魚肉!),鋼鐵的熱處理,鋼材的熱處理有退火、淬火(固溶化)以及回火(時效處理),退火是為了均質化、軟化鋼材以及消除應力,鋼鐵及鈦合金和少部份的銅合金可作麻田散相變態硬化(淬火+回火),淬火,將鋼材加熱至沃斯田鐵化溫度(亞共析鋼,Ac3,以上3060,共析及過共析鋼至,Ac1,以上3060),持溫30分/25,mm。,然後以水淬、油淬或風冷避開,S,曲線鼻端(波來鐵變態)而產生麻田散鐵或變韌鐵,而後放置於空氣中冷卻至室溫,可以達成鋼材的硬化。,回火,淬火後必須儘快回火,回火分為高溫回火以及低溫回火,高溫回火之回火溫度為500以上,可兼顧硬度以及韌性,回火至150200則稱為低溫回火,在消除淬火應力之下仍可保留相當高的硬度以及尺寸的安定,回火溫度愈高則持溫時間愈短,模具鋼、高速鋼等高合金鋼,一次回火無法完全消除殘留沃斯田鐵,也無法充分硬化,故須進行23次之回火,熱機處理,一般藉熱處理、塑性加工或添加合金元素來提高鋼材強度的方法,會降低鋼材的延性及韌性,加工熱處理(或稱熱機處理)是結合熱處理和塑加工之新製程,借由在變態溫度附近施以塑性加工,可在不降低延性、韌性的情況下,大幅提高強度,而成為超強韌鋼,最有名的例子有,TRIP,鋼、雙相鋼以及麻時效鋼,深冷處理,隨著鋼材的含碳量或淬火溫度升高,淬火回火後的殘留沃斯田鐵也會愈多,殘留沃斯田鐵會逐漸轉變為麻田散鐵而引起鋼材變形,稱為時效變形,淬火後繼續冷卻至室溫以下(-70 -190),麻田散鐵變態會更為完全,不但可避免日後的時效變形,也可大幅提高鋼材的硬度及耐磨性,表面硬化,各種機械用之軸、齒輪等,一方面要耐衝擊,另一方面軸之接觸部份或齒面,則必須具有耐磨耗之性質。為同時滿足此兩要求,唯有採用柔韌之鋼材,並施以表面硬化熱處理可以達到。,表面硬化之分類,物理性熱處理,但表面化學成份不變,化學性熱處理,但表面化學成份改變,被覆性表面鍍上硬質材料,機械性表面予以加工硬化,物理性表面硬化法,利用火焰、高週波、雷射甚至是太陽能將表面加熱(甚至重熔)產生淬火之效果,化學性表面硬化法,滲碳、氮化、滲硼利用擴散現象使硬化元素滲透進入金屬表層,並與鐵原子作用而產生硬化層,硫化、蒸氣、鉻化、鋁化利用化學友應在金屬表層產生一保護膜,被覆性表面硬化,濕式法電鍍硬鉻、溶膠凝法,可用於溫度不高之場合(壓鑄機車柱),乾式法加焊硬面法、碳化物被覆法、陶瓷披覆法,硬鍍以及鍍層附著性較高,可以用在高溫磨耗的場合(刀具以及壓鑄模),機械性硬化法,珠擊、噴砂、滾軋,材料表層受壓應力而產生加工硬化,可以提高疲勞性質,非鐵合金之熱處理,鋁合金、鎂合金以及大部份的銅合金之熱處理行為屬於時效硬化型,非鐵合金之熱處理分為3種:退火、固溶化以及時效硬化,退火(非鐵合金),退火可以軟化鋁材以利後續成形或加工,依目的可分為2種:,應力消除退火消除加工硬化,完全退火消除所有熱處理(尤其是析出硬化)的影響,固溶化+淬火,固溶化乃是加熱合金至,相固溶溫度以上,使合金成為均勻的,相。加熱溫度絕對不可以超過合金之共晶溫度以上,否則晶界會熔化導致合金脆化而無法復原,淬火乃是將合金從固溶化溫度迅速冷至室溫,使合金成為過飽和固溶體,作為後續時效應硬化的準備,時效硬化,過飽和的合金元素會以金屬間化合物的型態逐漸析出,剛開始是數量的增加,而後則伴隨著尺寸的成長,同時合金的強度以及硬度也開始增加,依其溫度可為為2種,自然時效在室溫下任其自然析出硬化,人工時效給予適當的溫度時間而析出硬化,當硬度達到最高值後開始下降則稱為過時效,熱處理對鋼材機械性質之影響,硬度、抗拉強度,疲勞特性,衝擊特性,耐磨性,切削性,硬度、抗拉強度(熱處理),熱處理鋼之硬度在,HB500,以下時,抗拉強度與硬度有以下關係:,(kgf/mm,2,)1/3HB,2.1HS 3.2HRc,鋼材之硬度視含碳量而定:,退火或正常化硬度,HB80+200*%C,淬火硬度,HRc 24+40*%C30+50*%C,回火硬度視回火溫度以及淬火完全性而定,疲勞特性(熱處理),材料的疲勞強度約為抗拉強度的4550%,而鋼材硬度為,HRc45,時疲勞強度最大(淬火不完全則疲勞強度劇降),由於疲勞損傷都是從表面開始,因此表面硬化熱處理可有效改善疲勞強度,衝擊特性,淬火、回火鋼之衝擊性最佳,但淬火完全性要高且回火溫度高,耐磨性,熱處理可有效提高耐磨性,其方式有3:,表面硬化熱處理,消除內應力,深冷處理消除殘留沃斯田鐵,切削性,切削性和成份、硬度有關。鋼材的成份對切削性的影響有一經驗公式:,切削性指數,M.I.,=265-600*%C-1300*%Si,-100*%Mn+100*%S+100*%Pb,最適於切削的硬度範圍是,HB185230(HRc21,以下),材料試驗,破壞性測試,金相(微結構)觀察,取樣金相切割機,鑲埋熱鑲埋機,研磨平面砂輪、水砂紙、雙盤研磨拋光機,拋光機械拋光、電解拋光,浸蝕化學腐蝕溶液,觀察金相顯微鏡、電子顯微鏡,金相切割機、熱鑲埋機,雙盤研磨拋光機,金相顯微鏡,硬度試驗,莫氏(劃痕)硬度,洛氏硬度(,HR,A,、HR,B,、HR,C,),勃氏硬度(,HB),維氏硬度(,Hv),微小硬度(,Hv、HK),蕭氏硬度(,HS),攜帶式硬度計:里氏硬度(,HL),超音波量測,洛氏硬度計,微小維氏硬度計,硬度轉換對照表,拉伸測試,拉伸試驗是一種最普遍、最早使用的材料試驗方法,標準試棒拉伸測試,產品拉伸測試(釘槍、,P79 frame,等),材料萬能試驗機,拉伸曲線,伸長量,力量,應變,應力,0.2%,降伏強度,抗拉強度,鋼鐵材料,塑膠,脆性材料,非鐵材料,疲勞試驗,材料受到重複施加的應力而斷裂,而每循環的應力強度皆小於該材料之降伏強度者,此種斷裂稱於疲勞斷裂,根據美國金屬學會(,ASM),統計,機械的斷裂中有8090%是材料疲勞的緣故,疲勞行為,S-N,曲線:,S,覆變應力,,N,疲勞生命週期,10,7,10,8,5*10,8,疲勞極限,非鐵金屬如鋁、鎂、銅等,不論應力如何降低,疲勞生命總有一定的極限,鐵、鈦等合金,在某一應力以下時,疲勞生命週期可達無限次,此一應力即稱為此材料之疲勞極限。工程上,假如材料在某一應力下週期次數達到10,7,次或10,8,次或者,5*10,8,次也不斷裂,其中最大應力當作疲勞極限,疲勞斷面,疲勞斷面壓鑄機車柱,疲勞斷面壓鑄機車柱,斷裂方向,疲勞性質影響因素,應力振幅、應力系統、溫度、頻率、應變振幅、晶粒大小、微結構、熱處理、表面效應(氮化、滲碳、高週波、噴砂脫碳、電鍍)、尺寸效應,其他材料試驗,衝擊試驗,壓縮試驗,彎曲試驗,扭力試驗,磨耗試驗,參考資料,工程材料科學,劉國雄等著,全華科技,熱處理,金重勳著,復文書局,北美壓鑄協會網站,www.diecasting.org,Federal Die Casting Company,網站,材料工程實驗與原理,林樹均等著,全華科技,
展开阅读全文